STATEMENT TILE REMODELING / REPLACEMENTS;
The adherence of tile or veneer products being applied during the re-tiling process of an existing swimming pool / spa and or water feature are subject to the status of the gunite shell's existing conditions. These conditions are unknown and outside the awareness of the current costs evaluations. Unknown conditions may exist that involve the effects of water saturation / penetration deterioration to the Bond Beam and or surfaces that are designated to have topical products reapplied. Repairs and remedy of such conditions are not part of any estimated costs assessments as they cannot be known until forensic investigation determines whether or not these will affect the re-applying process of the topical applications.
Therefore, until removal and discovery is performed of the existing underneath conditions, we cannot fully confirm that the intended work scope will not expand beyond the scope that’s been estimated. If this becomes a requirement an estimate will be submitted for approval prior to commencing with the additional repairs.
OPINION: The south east side of the pool concrete decking has lifted up approximately 1/2" to 3/4". It isn't definitively apparent as to why this has occurred including an original installation oversight in quality control.
Our logic here would be to eliminate the Redwood tree roots as a source, as the concrete's outer perimeter wall doesn't reflect a corresponding lifting.
Expansion and Contraction in Concrete Construction (PEI):
Most of us in the swimming pool construction industry know that many materials expand and contract with temperature change.
How many of us know how important proper trade practices are in minimizing problems due to temperature caused expansion and contraction, is another story?
For example, concrete is one of the most highly utilized materials in our industry today, yet the industry consistently sees swimming pools damaged by expansion and contraction of adjacent concrete flat-work.
The most important bit of information to remember is the expected expansion in concrete caused by temperature change. Between the heat of summer (pool deck surface at 130º to 140º) and the dead of winter (pool deck surface at 30º to 40º) we can expect at least a 100º temperature change.
The critical number to remember is that a 100 foot wide section of concrete will expand approximately 3/4 of an inch with a 100º temperature change. The expansion in lesser widths of concrete can be easily determined by proportioning the 3/4“ per 100 feet.
The force of expanding concrete is very high and can easily shear off the coping or bond beam without properly installed isolation joints.
Mastic Joints (PEI):
The mastic joint between the swimming pool concrete decking and the pool coping/bond beam is an extremely important component of a swimming pool and must be properly installed. The purpose of this joint is to isolate concrete deck movement from the pool coping/bond beam assembly.
As outlined above, concrete flat-work including pool decks expand and contract with temperature change (up to 100° of variation can be expected).
Without the installation (and proper maintenance) of a flexible mastic joint between the swimming pool decking and the pool coping, movement caused by expansion and contraction of the pool deck will frequently cause dislodged coping, tile and horizontal cracking in the water line tile, and in some cases lifting of the decking itself.
This mastic joint must extend the full depth of the concrete decking so that no portion of the concrete deck can apply pressure against the coping or any portion of the pool structure.
A design diagram (Construction Details) should be provided when proposing any replacements and or repairs in order to
direct proper construction joint techniques in order to not suffer future ramification from improper joint techniques.
As indicated in this narrative, an accompaniment of such a diagram establishes measurable standards that can come from design assistance. These efforts in turn define the clearer objective to be met from the responding solicitations, quoted pricing and performances from the selected Contractors.
In order to mitigate the potential of the dislodging of the pool coping, deck lifting / settling, horizontal cracking in the waterline tile and shearing of the bond beam from improper installation of the mastic joint, preparations need to be employed.
Proper installation of the mastic joint is normally the responsibility of the concrete pool decking installer and unfortunately this component of the swimming pool's construction has more to do with aesthetics than the building code compliance being critiqued by officials.
The lack of adequate maintenance of the mastic joint may result in a loss of expansion protection and can cause the same problems that are experienced without the installation of the mastic joint
.
Cantilevered Concrete Pool Decking (PEI)
Cantilevered concrete pool decking must also be properly installed to isolate concrete deck movement due to temperature expansion and other causes from the pool coping/bond beam assembly.
And again, the proper construction techniques basically requires the leveling of the top of the bond beam and then the installation of a bond breaker or slip joint on top of the leveled beam prior to pouring the concrete deck.
This can be shown on an accompanying diagram when plans are prepared By not following the proper construction techniques, the waterline tile may become partially applied to the cantilevered deck (which will result in horizontal cracks in the tile) or deck movement may shear off the leveling mortar course or the top of the bond beam.
Equipotential Bonding
No steel reinforcing should be extended from the bond beam into the pool deck. Further, the new cantilevered concrete deck should have no direct contact with the bond beam of the pool especially immediately behind the bond beam.
Bonding of the Leveling Course of Mortar
Reoccurring horizontal cracking and dislodging of the water line tile can also be caused by the un-bonding of the mortar or concrete layer used to level the top of the bond beam elevation prior to coping or cantilevered concrete deck application.
This un-bonding, most likely, has been caused by improper construction techniques used in the application of the mortar or concrete layer to the top of the lower bond beam elevation.
It is very important that correct procedures be followed to assure proper bond of this mortar course to the existing bond beam.
In order for a property Owner to become the beneficiary of such information, it is imperative that directions are provided for Contractors to follow.
"Construction Details" and design direction offer recommendations for how to approach the correct construction techniques.
City / County Building Inspectors are generally only concerned with attaining proper bonding of new materials such as masonry, tile, gunite and concrete to existing similar materials as that of being "code compliant".
Here are a few things that get missed absent the peripheral view's greater appreciation for the cause and effects mentioned above;
1. Existing surfaces must be sound, free of defects, clean and free of bond inhibiting materials.
2. Existing surfaces must be roughened by chipping or other suitable means to provide an open pore structure. All loose, cracked or deteriorated materials must be removed.
3. Clean existing surfaces by water blasting.
4. New material should be applied over cement paste or another approved bonding agent, which has been brushed onto the substrate (existing material) for absorption into the pore structure. The new material shall be applied before the cement paste or other approved bonding agent “skins over” or starts its “setting stage.”
5. Saturated surface dry condition of the substrate shall be maintained to prevent premature drying of the bonding paste.
Following these recommended practices will minimize problems in attaining proper bonding between these materials and will provide quality results.
* END OF NARRATIVE*
The mastic (Deck-O-Seal) material that has been applied in between the precast coping and the concrete decking fills a joint and this is a location that has the potential for water intrusion under the decking, especially if this mastic is not maintained to a good standing periodically.
It is apparent that the mastic needs some attention / repair and it would be our recommendation to remove the old mastic material and re-apply it per the MFG.'s directions.
|